bruce-zhou-avator-600x600

Written by Bruce Zhou
Founder & Managing Director | JOTA Machinery
Paper converting machinery specialist since 2002.
Connect with me on LinkedIn
Published: 21,October, 2026
Last Updated: 21,October, 2026 15:39:40 PM GMT+8

The thermal paper rolls have just passed through the shrink wrapping machine. The sealing process looks normal, and the packages have travelled through the heat shrink tunnel.

However, the finished packages don’t look right.

The plastic film is loose around the thermal paper rolls. Wrinkles remain on the surface, the corners are not properly formed, and some rolls can move slightly inside the wrapping.

The operator increases the shrink tunnel temperature, hoping to make the film tighter.

The packaging improves, but another problem appears: the thermal paper begins to turn grey or black because of excessive heat exposure.

This is a common challenge when packaging heat-sensitive products such as POS receipt rolls and thermal till rolls.

Unlike ordinary products that can tolerate greater heating, thermal paper has a heat-sensitive coating. Excessive exposure to the hot air inside a shrink tunnel can cause unwanted colour development.

The goal is therefore not simply to make the shrink film tighter by increasing the temperature.

The goal is to obtain a neat, secure shrink package without overheating the thermal paper underneath.

If the shrink film remains loose, the problem may involve film dimensions, shrink properties, conveyor speed, hot air distribution, sealing conditions or the arrangement of the finished rolls.

This guide explains how to investigate loose shrink wrapping on thermal paper rolls and how to improve packaging quality without causing heat damage.

1. First, Identify Where the Shrink Film Is Loose

Before adjusting the packaging machine, examine the finished package.

Not all loose shrink wrapping defects have the same cause.

shrink-pack-750x563

A package that is loose across its entire surface may require a different correction from one that has wrinkles only around the ends.

Loose Film Around the Entire Package

If the film remains loose on most surfaces, the shrink process may not be providing the required film contraction.

Possible causes include insufficient heat exposure, an unsuitable film grade or a film sleeve that is too large for the product.

Wrinkles Around the Roll Ends

If the main surfaces are reasonably tight but wrinkles remain around the ends, check the film dimensions, sealing position and airflow distribution.

Excess material may be gathering where the film cannot contract neatly around the package geometry.

One Side Tight, the Other Side Loose

This may indicate uneven heating, incorrect product positioning or airflow differences inside the tunnel.

The film may be shrinking more effectively on one side than the other.

Rolls Move Inside the Package

If the individual thermal paper rolls can shift inside a completed pack, examine the initial grouping arrangement and the finished film fit.

The problem may begin before the product enters the tunnel.

Excessive clearance between the rolls and the sealed film can remain even after shrinking.

Practical advice: Identify the exact defect before changing the tunnel temperature. The appearance and location of the loose film provide useful clues.

2. The Shrink Film Is Too Large for the Thermal Paper Rolls

An oversized shrink film sleeve or bag is one of the first things worth checking.

During shrink wrapping, the film must have sufficient space to pass around the product and form a proper seal.

However, excessive film width or cut length can leave more material than the shrink process can accommodate neatly.

shrink-rolls-750x563

The result may be loose surfaces, large folds or protruding film at the package ends.

Why Film Dimensions Matter

Suppose the manufacturer changes from packaging larger POS rolls to smaller card machine rolls.

The same film width and cut length may no longer be suitable.

If the packaging machine continues feeding the original amount of film, the smaller rolls may enter the shrink tunnel with excessive material around them.

The tunnel can shrink the film, but it cannot necessarily produce a neat package from an incorrectly sized sleeve.

How to Correct the Problem

Measure the actual dimensions of the roll or group of rolls being packaged.

Then review the required film width, bag length and sealing position according to the wrapping machine’s film-sizing method.

Reduce unnecessary excess material while maintaining sufficient clearance for feeding and sealing.

Check the results using several test packages.

Do not make the film so small that it stretches excessively before sealing or places unacceptable pressure on the finished rolls.

Why This Should Be Checked Before Increasing Heat

If the original film dimensions are incorrect, raising the tunnel temperature may improve the appearance slightly but may not eliminate the folds.

For thermal paper rolls, the additional heating also increases the risk of darkening the sensitive coating.

Correcting the film dimensions may be a more effective first step.

3. Shrink Tunnel Temperature Is Too Low for the Selected Film

If the film dimensions are correct but the package remains loose, examine whether the film is receiving sufficient heat to shrink.

Polyolefin shrink film is designed to contract when exposed to appropriate processing conditions.

However, different film grades have different shrink characteristics.

If the tunnel temperature is below the effective operating range for the selected film, the material may not achieve the intended shrinkage.

Typical Symptoms

  • Film remains loose across large areas.
  • Wrinkles are visible after the tunnel.
  • The film does not conform to the roll surfaces.
  • Corners or ends remain poorly formed.
  • Packaging appearance varies with production conditions.

These symptoms can also result from insufficient exposure time or airflow.

Why Increasing Temperature Is Risky for Thermal Paper

With ordinary products, an operator may try a moderate temperature increase.

For thermal paper rolls, this must be approached carefully.

The paper’s heat-sensitive coating may darken if the product receives excessive heat.

A tunnel temperature that shrinks the film satisfactorily may still be unsuitable for the paper.

Therefore, the operator should review the film’s specified shrinking conditions and the tunnel’s actual performance before increasing the temperature.

If a conventional film requires excessive heat, a different film grade may be necessary.

4. Conveyor Speed Is Too Fast

The conveyor determines how long each package remains in the heated section of the shrink tunnel.

If the conveyor travels too quickly, the film may leave the tunnel before receiving sufficient thermal energy.

The package may appear partially shrunk but remain loose in certain areas.

How to Investigate

Confirm the current conveyor speed and the approximate residence time inside the heated section.

Observe whether the same film shrinks more effectively under a slightly longer permitted exposure.

Where the equipment manufacturer allows it, perform a controlled trial with a small conveyor-speed adjustment.

Keep the other parameters unchanged so that the result can be evaluated.

Why Slowing the Conveyor Can Create Another Problem

Slower movement gives the film more time to shrink.

It also gives the thermal paper more time to absorb heat.

This can result in discolouration even if the tunnel temperature remains unchanged.

For this reason, operators should not continue reducing conveyor speed until the film becomes tight without checking the paper inside.

The correct packaging setting must satisfy both film shrinkage and thermal paper protection.

Important: Tunnel temperature and conveyor speed should be evaluated together, but changed systematically rather than randomly.

5. Hot Air Distribution Is Uneven Inside the Shrink Tunnel

Shrink film needs suitable heat distribution to contract around the package.

If one side receives more heat than another, the film may shrink unevenly.

This can leave wrinkles, loose corners or differences in film tightness across the package.

What Can Cause Uneven Heating?

Depending on the tunnel construction, possible causes include:

  • Blocked or incorrectly positioned air outlets
  • Improper airflow settings
  • Poor product positioning
  • Uneven distribution of packages on the conveyor
  • Abnormal circulation fan operation
  • Hot or cold zones inside the tunnel

How to Identify an Airflow Problem

Look for a consistent pattern.

For example, if packages are always loose on the same side, investigate whether that side receives sufficient heated airflow.

If the problem appears mainly with wider packages, examine whether the tunnel provides suitable air circulation around the entire product.

Also check whether packages are entering the tunnel too close together, potentially affecting the airflow around each pack.

How to Correct It

Inspect the tunnel’s circulation system according to the machine manufacturer’s maintenance instructions.

Check air outlets and confirm the approved airflow configuration.

Make sure the packages enter the tunnel in the intended orientation and spacing.

If adjustments are available, perform a controlled trial within the equipment’s permitted operating range.

Do not open guarded hot-air sections or modify heater components while the equipment is running.

For thermal paper rolls, uniform heat distribution may help achieve acceptable shrinkage without relying on unnecessarily high temperatures.

6. The Shrink Film Has Unsuitable Shrink Properties

Sometimes the problem is not the machine adjustment.

The selected film may not be suitable for the product and packaging conditions.

Different shrink film grades have different shrinkage curves, shrink-force characteristics and processing windows.

A film that performs satisfactorily on another packaged product may not be ideal for thermal paper rolls.

What Should Be Checked?

Review the material specifications, particularly:

  • Film material and grade
  • Film thickness
  • Shrinkage behaviour at different temperatures
  • Machine-direction and transverse-direction shrinkage
  • Shrink force, where relevant
  • Recommended sealing conditions
  • Recommended tunnel operating conditions

The relationship between shrinkage in the machine direction and transverse direction matters when the film must conform to a particular package shape.

If the film contracts differently from what the package geometry requires, wrinkles or uneven fit may remain.

Consider Low-Temperature POF Shrink Film

For thermal paper rolls, low-temperature polyolefin (POF) shrink film is worth evaluating.

Certain specially formulated grades, including low-temperature cross-linked polyolefin shrink film, can provide useful shrinkage at relatively low heating conditions.

This may allow the manufacturer to improve film fit without exposing the thermal paper to excessive heat.

However, not every POF film or cross-linked film is a low-temperature grade.

The selected product must be verified using the supplier’s technical data and actual packaging trials.

What If the Film Still Remains Loose?

If the film has suitable low-temperature shrink properties but the package remains loose, inspect film sizing, airflow and sealing before increasing heat exposure.

Changing the film alone will not correct an oversized bag or a poorly configured tunnel.

7. Trapped Air Prevents the Film From Fitting Properly

During heat shrink wrapping, air can become trapped inside the sealed film.

As the package enters the tunnel, this trapped air may expand and make the film balloon away from the product.

If the air cannot escape in a controlled way, the package may develop wrinkles, loose areas or an inflated appearance.

How to Recognise Trapped Air

The film may expand noticeably during heating.

After cooling, loose pockets or folds may remain.

The problem can be more visible with certain package shapes or larger bundles.

How to Correct It

Check the packaging machine’s air-evacuation arrangement.

Some shrink wrapping systems use suitably positioned perforations or other controlled venting methods.

Where such a system is provided, inspect whether it is operating correctly.

Verify that the film type and package format are compatible with the intended venting arrangement.

Do not add arbitrary holes to the film without considering the required packaging protection, seal integrity and machine design.

A correctly configured air-release system can help the film settle around the product during shrinking.

8. Incorrect Sealing Position or Weak Seals

The shrink tunnel cannot compensate for every defect created at the sealing station.

If the film is cut or sealed with excessive clearance, the completed package may retain unnecessary material.

If the seal is weak or partly open, the package may not retain its intended shape.

What Should Be Inspected?

Check the sealing position relative to the packaged thermal paper rolls.

Inspect the seal for gaps, damage, contamination or inconsistent bonding.

Verify the sealing temperature, contact pressure and sealing cycle according to the film and equipment specifications.

If the machine has a sealing blade or wire, inspect its condition using the prescribed maintenance procedure.

Loose Film vs Weak Seals

These problems should be distinguished.

A loose package may have strong, properly formed seals but insufficient shrinkage.

A package with weak seals may open or separate during heating and handling.

Increasing tunnel temperature is not a reliable correction for an improperly formed seal.

The sealing process should be corrected at its source.

9. The Thermal Paper Rolls Are Not Grouped Correctly

When several finished thermal paper rolls are packaged together, the position of each roll affects the shape of the bundle.

If the rolls are not properly grouped before wrapping, the resulting pack may contain gaps or uneven surfaces.

The shrink film then contracts around an unstable product arrangement.

This can create an irregular package even when the film and tunnel are operating correctly.

Example: Multiple Thermal Receipt Rolls in One Pack

Suppose a packaging line wraps several small receipt rolls together.

If the rolls are aligned evenly and remain in the intended arrangement during sealing, the film can contract around a more consistent shape.

If some rolls shift or become separated before entering the tunnel, the film may shrink around the gaps.

After cooling, the package may appear loose or distorted.

How to Improve the Result

Check the product grouping and positioning before wrapping.

Confirm that the rolls remain appropriately aligned during film feeding, sealing and transfer into the tunnel.

If the packaging machine includes product guides or grouping mechanisms, verify their adjustment for the specific roll dimensions.

Avoid trying to correct poor grouping simply by increasing shrink force or heating.

Excessive shrink force can deform a soft product without resolving the original alignment problem.

10. Quick Troubleshooting Guide for Loose Shrink Wrapping

When finished thermal paper roll packages are too loose, the operator should inspect the most likely causes in a consistent order.

Observed DefectPossible CauseFirst Action
Entire package is looseInsufficient shrinkage or oversized filmCheck film dimensions and shrink specification
Large folds at the endsExcess film or incorrect bag lengthReview cut length and sealing position
One side is looseUneven airflow or positioningCheck tunnel airflow and product alignment
Film balloons during heatingTrapped airInspect approved venting arrangement
Film loose after high-speed operationInsufficient residence timeReview conveyor speed and shrink performance
Package opens during shrinkingWeak or damaged sealInspect the sealing station
Film is tight but paper turns blackExcessive heat exposureReduce thermal load and review film grade
Rolls move inside the packExcess clearance or unstable groupingCheck initial grouping and film sizing
Wrinkles persist despite increased heatFilm mismatch, poor sizing or uneven airflowStop increasing temperature and investigate setup

The table is a starting point for diagnosis.

More than one factor may contribute to a packaging defect.

For example, an oversized film sleeve and insufficient airflow can produce similar-looking loose areas.

The operator should identify the original cause before making major adjustments.

11. A Practical Adjustment Procedure for the Packaging Line

A useful troubleshooting method is to evaluate the package before, during and after shrinking.

Step 1: Inspect the Package Before the Tunnel

Check the film dimensions, cut length, sealing position and product grouping.

If the package is already excessively loose before heating, correct the wrapping arrangement first.

Step 2: Inspect the Shrink Film

Confirm the exact film grade and thickness.

Review the supplier’s recommended shrinking conditions.

If the thermal paper is heat-sensitive, determine whether a suitable low-temperature film is available.

Step 3: Check the Tunnel Setup

Record the current temperature setting, conveyor speed and airflow configuration.

Allow the equipment to reach stable operating conditions before testing.

Step 4: Run a Small Test Batch

Process a small number of representative packages.

Inspect whether the film contracts evenly and whether the thermal paper remains undamaged.

Step 5: Change One Variable at a Time

If the package remains loose, use the observed defect to decide which setting or component to investigate.

For example, inspect the film size if large folds remain at the ends.

Check airflow if one side is consistently loose.

Review tunnel exposure if the film is uniformly under-shrunk.

Step 6: Inspect the Rolls After Cooling

Check the finished film appearance, seal integrity and product condition.

For thermal paper rolls, inspect the heat-sensitive surface for grey or black discolouration.

A tight package should not be accepted if the paper has been damaged.

Step 7: Record the Approved Settings

Once satisfactory results have been achieved, record the film specification and machine conditions.

Repeat the trial over a representative production run to confirm that the packaging quality remains consistent.

The approved setup can then serve as a reference for future batches of the same product.

12. Why More Heat Is Not Always the Correct Solution

For many products, shrink wrapping problems are addressed by adjusting temperature or conveyor speed.

Thermal paper requires greater care because the product itself responds to heat.

An operator may achieve a visually perfect package by increasing tunnel temperature, only to discover that the receipt paper inside has darkened.

This creates a conflict between packaging appearance and product quality.

The correct approach is to identify a suitable processing window.

Within this operating range, the film should shrink sufficiently while the thermal paper remains acceptable.

A suitable low-temperature POF shrink film may help widen the available processing window by allowing shrinkage under reduced heat exposure.

However, the result still depends on film dimensions, package geometry, airflow, conveyor speed and sealing conditions.

What Should a Successful Trial Demonstrate?

The finished package should have:

  • Acceptable film tightness and appearance
  • No excessive wrinkles or loose ends
  • Intact seals
  • Stable arrangement of the packaged rolls
  • No unacceptable deformation of the products
  • No unwanted thermal paper darkening
  • Acceptable thermal printing performance after packaging

These requirements should be established before approving the packaging process for regular production.

13. Preventing Loose Shrink Packages in Daily Production

Once the line has been properly adjusted, repeatability becomes important.

A setup that works for one thermal paper roll size may not work for another.

Changing from larger POS rolls to smaller card machine rolls can affect film requirements, packaging dimensions and tunnel exposure.

Likewise, changing the number of rolls in each pack can alter the product geometry.

Operators should therefore verify the setup whenever the packaging format changes.

A useful production record includes the thermal paper roll specification, package quantity, film grade, film width, cut length, sealing parameters, conveyor speed, tunnel settings and inspection results.

Routine maintenance also helps prevent quality variation.

Inspect the film feeding system, sealing components, conveyor movement and tunnel air circulation according to the equipment manufacturer’s schedule.

If loose packaging begins appearing after a previously stable production period, compare the current machine and material conditions with the approved setup before making adjustments.

Conclusion: Tight Packaging Without Overheating Thermal Paper

Loose shrink wrapping on thermal paper rolls can result from several different problems.

The film may be too large for the package, the shrink tunnel may not provide sufficient or even heating, the conveyor may be moving too quickly, or trapped air may prevent the film from fitting correctly.

Weak seals and unstable roll grouping can also contribute to poor package appearance.

Although increasing tunnel temperature may improve shrinkage, it is not always the right solution for heat-sensitive thermal paper.

Excessive heating can activate the paper’s thermal coating and turn the finished rolls grey or black.

For manufacturers experiencing this problem, the best approach is to begin with film dimensions, product grouping and sealing quality before reviewing tunnel conditions.

Where the selected film requires excessive heating, a suitable low-temperature POF shrink film, including an appropriately formulated cross-linked grade, may provide a better alternative.

The final goal is not simply a tighter plastic film.

It is a secure, consistent package that protects the thermal paper rolls throughout handling, storage and distribution.

Planning a Thermal Paper Roll Production and Packaging Line?

JOTA Machinery manufactures thermal paper slitting and rewinding equipment and provides production-line solutions for finished POS receipt rolls and thermal till rolls.

If you’re planning a converting line with downstream shrink wrapping, the finished roll dimensions, packaging arrangement and thermal paper sensitivity should be considered together.

900A-slitter-rewinder-machine-1125x750

Need to increase thermal paper roll production while reducing manual handling? The JT-SLT-1400FA integrates automatic core feeding, slitting, rewinding, and finished roll handling into a connected production line. During normal operation, one operator can supervise and inspect the production process. For manufacturers handling large-volume POS and receipt roll orders, our team can discuss production capacity, automation requirements, and suitable downstream packaging configurations.

Share your jumbo paper specifications, finished roll sizes, packaging quantity and expected production capacity with our engineering team.

We can discuss suitable converting and packaging-line requirements and the production tests needed to evaluate the complete process.

Discuss Your Thermal Paper Production and Packaging Requirements

Last Updated on 21/10/2026 by Jota Machinery

Scroll to Top